The most common problems encountered in overmolding are:
	- Poor adhesion
- Incomplete filling of the substrate or overmold
- Flashing of the overmold
Corrective actions for many of these problems are presented below.
	
		
			| Observation | Possible Causes | Corrective Actions | 
	
	
		
			| Flash (over substrate or on periphery of part) | 
				Poor mold fitInadequate molding machine tonnagePoor shutoff designSubstrate shrinkage | 
				Check by bluing the toolIncrease tonnage or decrease injection and pack pressureRe-cut tool to obtain complete shutoffCheck for substrate sinks and re-cut tool | 
		
			| Short shots | 
				Not enough materialNot enough injection pressureNot enough fill speedMelt too coldPoor venting | 
				Increase shot sizeIncrease injection pressureIncrease injection speedIncrease melt temperatureDecrease the clamp tonnage and re-cut vents | 
		
			| Poor quality knit lines | 
				Gas trapped between polymer frontsLow melt temperature | 
				Improve ventsIncrease injection speed and melt/mold temperature | 
		
			| Overmold breaks or impinges through hollow substrate | 
				Improperly supported substrateHigh injection pressure and melt temperatureWrong location of gate | 
				Fully support the substrate to resist hydraulic injection pressures and meltingLower injection pressure and melt temperatureRelocate gate | 
		
			| Warped parts |  | 
				Lower the molded in stress in both the substrate and the elastomerIncrease the stiffness of the substrate by including glass or increasing thickness of ribs | 
		
			| Poor adhesion | 
				Incompatible materialsContaminationGate freeze-off too early | 
				Re-select correct grade of TPECheck for color concentrate compatibility and/or the use of a lubricated grade of substrateIncrease the process temperatures and/or mold temperature | 
		
			| Surface sinks | 
				Material shrinkage causes non-uniform release from tool surfaceGate freeze-off too early | 
				Increase the pack pressure/hold time and decrease material temperatureIncrease gate size | 
		
			| Non-uniform color | 
				Incompatible color concentrateInadequate melting and dispersion of color concentrate | 
				Check for concentrate compatibilityIncrease rear zone temperature, back pressure, screw RPM | 
		
			| Surface splaying (silver streaking) |  |  | 
		
			| Parts stick in the "A" side of the tool | 
				Not enough draftPart forms a vacuum in the "A" cavity"A" cavity too shiny"A" cavity too hot | 
				Increase the draftProvide air assist releaseSandblast the cavityRun the "A" half cooler | 
		
			| Elastomer is sticky or smells |  | 
				Check for material residence time and reduce temperature in rear zones if possible |